Home-Knowledge-

Content

Upgrading from DC04 to DC07 for Complex Deep Drawing

Dec 05, 2025

Two Grades, Two Forming Categories

Under EN 10130 the cold rolled forming family progresses from DC01 for bending through DC03 for drawing, DC04 for deep drawing and up to DC05, DC06 and DC07 for increasingly severe operations. DC04 is the workhorse deep drawing grade: it produces appliance panels, automotive brackets and general stamped components reliably, and it is available from every mill at a competitive price. DC07 is a different category. It is a stabilised ultra deep drawing grade with a typical yield strength limit of 150 MPa maximum, a tensile range of 250 to 310 MPa and a minimum elongation of 44 percent, supported by a plastic strain ratio of 2.5 minimum and a strain hardening exponent of 0.230 minimum. Those figures, not the grade label, describe what the material can survive.

The Mechanical Gap

Property DC04 DC07
Standard EN 10130 EN 10130
Forming category Deep drawing Ultra deep drawing
Yield strength Re 140-210 MPa 150 MPa max.
Tensile strength Rm 270-350 MPa 250-310 MPa
Elongation A80 min. 38 % 44 %
Plastic strain ratio r90 min. Higher than basic drawing grades 2.5
Strain hardening exponent n90 min. Suitable for standard draws 0.230

The gap that matters most in a difficult die is the r90 value. A higher plastic strain ratio means the material resists thinning when it is stretched over a punch, so the wall of the cup stays thicker and the blank can be drawn deeper before the wall fractures. Higher n90 adds even strain distribution and delays local necking. A low yield strength reduces the punch force needed and reduces springback, which simplifies die tryout. The combination is what allows DC07 to complete a draw that DC04 fails at the bottom radius.

Where the Upgrade Pays

Multi-stage sequences that combine drawing, redrawing, flanging and ironing, where each stage consumes some of the remaining ductility of DC04.

Parts with steep walls and tight punch radii, where thinning becomes critical before the full depth is reached.

Components with a large draw ratio relative to blank diameter, where the blank must flow a long distance into the die cavity.

High volume runs where a small reduction in cracking saves more than the material premium through lower scrap and fewer stoppages.

Parts painted, galvanized or electroplated after forming, where a smoother surface reduces coating consumption and improves finish uniformity.

Tooling and Process Effects

Moving to DC07 changes the process window rather than only the material. Lower yield strength means lower blank holder force is needed for the same restraint, so press settings from a DC04 trial will usually need to be reduced; leaving them unchanged produces wrinkles instead of tears. Die clearances remain in the usual range for mild steel of about 8 to 12 percent of thickness per side, but the reduced springback allows a less aggressive overbend in the die face. Lubricant selection becomes more important because the drawn surface area is larger and the contact pressure is lower; an oil that performed adequately with DC04 may need to be replaced with a higher film strength grade. Material model parameters for forming simulation must be updated with the r90 and n90 values measured on the actual coil, since simulations run with generic values mispredict the drawable depth for ultra deep drawing grades.

Quality Control When Switching Grades

The switch is normally controlled by a first article trial followed by dimensional and thickness inspection at the critical wall section, because thinning rather than cracking is the failure mode that passes casual inspection. Suppliers should provide inspection documents to EN 10204 type 3.1 with tensile results to EN ISO 6892-1 and r and n values determined to ISO 10113 and ISO 10275, so that the arrival condition of each coil can be compared with the trial material. Coil to coil consistency matters in a high volume press line: a narrow band on yield strength and elongation keeps the die setting stable across the order. Storage is also part of control, because stabilised grades such as DC07 do not age, and a press shop that has previously suffered from the erratic behaviour of ageing grades will notice the difference in long campaigns.

Frequently Asked Questions

Q: Is DC07 always better than DC04?

A: Only when the part needs it. For conventional deep drawing DC04 is adequate and significantly cheaper.

Q: What is the yield strength difference?

A: DC04 is specified from 140 to 210 MPa, while DC07 is limited to a maximum of 150 MPa, which reduces press load and springback.

Q: Why do wrinkles appear after switching to DC07?

A: The lower yield strength means the blank holder force must be reduced; keeping the previous DC04 setting over-restrains the blank edge.

Q: Does DC07 need a different lubricant?

A: Often yes. The larger drawn area and different contact conditions may require an oil with higher film strength.

Q: What values should be on the certificate?

A: Tensile results to EN ISO 6892-1 plus r90 to ISO 10113 and n90 to ISO 10275, since forming simulation depends on them.

SEND INQUIRY