What Galvanized Coating Quality Testing Measures
On galvanized steel sheet, coil and fabricated parts, coating quality is defined as the amount of zinc deposited per unit area of steel surface. It is expressed either as coating mass in grams per square metre or as coating thickness in micrometres. The two units are linked by the density of zinc, which gives a working conversion of approximately 1 micrometre of coating to about 7.1 g/m2 on one surface. Because that conversion is fixed, a mill can report either unit and the inspection certificate remains comparable between suppliers.
Coating mass figures are normally stated for both surfaces combined, following the convention of EN 10346 and ASTM A653. A Z275 coating therefore means 275 g/m2 in total, equivalent to roughly 137 g/m2 and 19 micrometres per side. Whether a stated figure is per side or in total is one of the most frequent causes of specification disputes in export contracts, so the unit and the basis should always appear on the mill certificate and in the enquiry.
The Gravimetric Dissolution Method: GB/T 1839, ISO 1460, ASTM A90
Chemical dissolution, also called the gravimetric method, is the reference technique for coating mass. GB/T 1839, ISO 1460 and ASTM A90 describe the same principle: the coating is stripped in inhibited acid, and the mass loss divided by the coated area gives the coating mass.
Degrease and clean the specimen, then dry it completely before weighing.
Prepare the inhibited solution by dissolving 3.5 g of hexamethylenetetramine in 500 mL of concentrated hydrochloric acid of density 1.19 g/mL, then dilute to 1000 mL with distilled water.
Immerse the specimen fully and let the reaction continue until hydrogen evolution stops distinctly.
Remove, rinse, dry and reweigh; coating mass equals the mass difference divided by the coated surface area.
At least two parallel specimens are tested and the mean value is reported. Specimens should be taken from flat, unworked areas away from sheared edges, where coating may be thinned or mechanically damaged. Because the method destroys the sample, it is used for referee testing and periodic process verification rather than for routine coil-by-coil sorting.
Non-Destructive Measurement: XRF, Magnetic and Eddy Current Gauges
X-ray fluorescence to ISO 3497 measures coating mass without damaging the strip and is widely installed on continuous galvanizing lines, where it provides a running record along the coil length. Magnetic thickness gauges to ISO 2178, together with the eddy current techniques covered by ASTM E376, give rapid local readings on finished sheet, tube and structural parts. These instruments are calibrated against certified reference foils or against gravimetric results, and their readings are reported on the same coating mass basis that was agreed with the customer.
Non-destructive methods are fast and can map the whole coil surface, but they are comparative. Where a contract specifies a coating mass with legal weight, the gravimetric result governs and the gauge is used for process control between referee tests.
Sampling and Acceptance: ISO 1461, EN 10346, ASTM A653
For hot-dip galvanized fabricated articles, ISO 1461 defines reference areas and the minimum number of measurements according to article length and batch size. Its default coating classes give a minimum average and local thickness: 85 micrometres average and 70 local for steel 6 mm and thicker, 70 and 55 for 3 mm to below 6 mm, 55 and 45 for 1.5 mm to below 3 mm, and 45 and 35 below 1.5 mm.
| Product | Standard | Designation basis |
|---|---|---|
| Hot-dip galvanized articles | ISO 1461 | Minimum average and local coating thickness |
| Continuously galvanized sheet | EN 10346 | Z classes from Z100 to Z600, total coating mass |
| Continuously galvanized sheet | ASTM A653 | G designations, G90 equals 0.90 oz/ft2 total |
G90 in ASTM A653 corresponds to about 275 g/m2 total, which is the same basis used for the European Z275 class. Buyers who work with both systems should convert to g/m2 before comparing offers.
Process Control, Inspection and Delivery Documentation
Coating quality is held stable by controlling line speed, bath chemistry, strip temperature and air-knife pressure, and by measuring coating mass at the start, middle and end of every coil. Weld zones, coil ends and strip edges receive additional attention because coating weight varies there. For export orders, the inspection certificate issued to EN 10204 3.1 records the specified class, the measured values and the test methods used. Adhesion is checked separately by bending or impact tests, and surface condition is agreed to a defined appearance grade, since a coating that meets the mass requirement can still be rejected for spangle, streak or edge build-up.
Frequently Asked Questions
Q: What is the difference between coating mass and coating thickness?
A: Coating mass is measured in g/m2 and coating thickness in micrometres. They are related by the density of zinc, so about 1 micrometre equals roughly 7.1 g/m2 on a single surface.
Q: Which test method is the reference for coating mass?
A: Gravimetric dissolution to GB/T 1839, ISO 1460 or ASTM A90 is the reference method, because it removes the coating and measures the mass directly.
Q: Can XRF replace gravimetric testing?
A: XRF to ISO 3497 is excellent for routine and in-line control, but it is calibrated against gravimetric values, so the dissolution method remains the referee test in disputed cases.
Q: How many measurements does ISO 1461 require?
A: ISO 1461 sets reference areas and a minimum number of readings that increase with article length and batch size, with acceptance judged on both average and local minimum thickness.
Q: What does Z275 mean on a galvanized coil?
A: It means 275 g/m2 of zinc in total on both surfaces, which is about 137 g/m2 and 19 micrometres per side.
Q: Why does coating mass matter beyond corrosion life?
A: Heavy coatings can crack or flake during tight bending and forming, so the coating class must match the forming severity as well as the required service life.