DIN EN 10130 Cold-Rolled Steel: Grades and Selection Guide

Dec 01, 2025

What DIN EN 10130 Covers

DIN EN 10130 is the German national adoption of EN 10130, titled Cold-rolled low-carbon steel flat products for cold forming. It specifies grades for cold-rolled uncoated steel in thicknesses up to 6 mm, delivered as coil, slit strip, or sheet. The standard defines the designation system, the mechanical properties, the surface quality classes, and the testing rules. Because it is a harmonized European standard, the same text is published in all member states; DIN EN 10130 and EN 10130 refer to the same document.

The Grade System DC01 to DC07

The grade name starts with DC, which stands for drawing-quality cold-rolled steel. The digits indicate the forming capacity, which increases with the number: DC01 is the general forming grade, DC03 and DC04 are drawing grades, DC05 is a deep-drawing grade, DC06 is an extra-deep-drawing grade, and DC07 is an ultra-deep-drawing grade produced as an interstitial-free steel. As the grade number rises, the maximum yield strength falls and the minimum elongation rises, which is the direct measure of formability.

Grade Max Yield Re (MPa) Tensile Rm (MPa) Min Elongation A80 (%) Typical Use
DC01 280 270 - 410 28 General forming, simple bending
DC03 240 270 - 370 34 Light drawing and stamping
DC04 210 270 - 350 38 Deep drawing
DC05 180 270 - 330 40 Deep drawing, complex shapes
DC06 170 270 - 330 41 Extra-deep drawing
DC07 150 250 - 310 44 Ultra-deep drawing, extreme forming

Values are the standard requirements for the delivered condition. DC07, for example, is an interstitial-free steel suitable for difficult deep-drawing and stretch-forming parts such as side walls, oil pans, and bottom plates, because it keeps a very low yield strength and high elongation.

Why Cold-Rolled Steel Is Used

Cold rolling reduces the strip at room temperature after pickling of the hot-rolled base, which imparts precise mechanical properties, a smooth surface finish, tight gauge tolerance, and good strip shape. Cold-rolled sheet performs excellently in deep drawing and intricate bending, welds easily, and offers a uniform surface that is simple and economical to finish or paint. Higher-strength cold-rolled grades are used where weight reduction, strength, and durability are required in the same part.

Typical Delivery Capabilities

Parameter Typical Range Remark
Thickness 0.30 - 3.00 mm Common cold-rolled range; thinner and thicker by arrangement
Width 600 - 1850 mm Depends on the mill and the order
Delivery forms Coil, slit strip, cut-to-length sheet Per the product standard
Surface quality Classes per EN 10130 State the class on the order

Size capability varies by facility, so the exact available range should be confirmed with the supplier for each order.

Mapping to Other Standards

EN 10130 grades are often compared with designations in other systems. The table below gives common references; exact equivalence depends on the property requirements, so each standard should be checked directly.

EN 10130 JIS G3141 ASTM A1008/A1008M SAE J403 / J2329
DC01 SPCC CS 1006 - 1010 / CR1
DC03 SPCD DS CR2
DC04 SPCE DDS CR3
DC05 SPCF EDDS CR4
DC06 SPCG EDDS (IF) CR5
DC07 SPCG (IF) EDDS (IF) CR5

Other cold-rolled specifications cover related products: enamelling steels are specified in their own standards for porcelain-enamelled parts, and high-strength cold-rolled grades are covered by standards such as EN 10268 or the automotive material systems rather than by EN 10130.

FAQ

Is DIN EN 10130 the same as EN 10130?

Yes. DIN EN 10130 is the German edition of the identical European standard EN 10130. The content, grade designations, and requirements are the same.

What does the grade number in DC01 mean?

The letters DC identify drawing-quality cold-rolled steel. The digits order the grades by increasing formability; higher numbers have lower yield strength and higher elongation and are used for deeper drawing operations.

Can EN 10130 grades be galvanized?

Yes. DC grades are common substrates for hot-dip galvanizing on continuous lines; the coated products are then designated under EN 10346, for example DX51D or DX53D. The drawing qualities of the EN 10130 family carry over into the coated product range.

What is the thickness range of EN 10130 sheet?

EN 10130 applies to cold-rolled flat products up to 6 mm thickness. In practice most orders are in the 0.3 to 3.0 mm range, and the tolerances are given in EN 10131.

Which grade is best for an oil pan or side wall?

Deep-drawn parts such as oil pans, side walls, and bottom plates are typically made from DC06 or DC07, which provide the very low yield strength and high elongation that these extreme forming operations require.

What documents confirm the grade on delivery?

The mill test certificate records the grade, heat and ladle analysis, mechanical test results, and dimensions. It is the reference for verifying that the delivered material meets the EN 10130 requirements of the order.

SEND INQUIRY