Why Aluminium and Magnesium Are Added to Zinc
A pure zinc coating protects steel in two ways: it acts as a barrier and it sacrifices itself at exposed steel. Alloy additions improve both functions. Aluminium forms a more stable oxide layer that slows the anodic dissolution of zinc, and magnesium stabilises the corrosion products into a dense, adherent layer that keeps protecting the cut edge after the initial zinc has been consumed.
In naming convention the elements appear in order of amount, so zinc-aluminum-magnesium means a zinc-based coating with small additions of aluminium and magnesium, while aluminum-zinc describes an aluminium-based coating with a zinc addition. That naming logic explains why the two families behave so differently in service even though they contain the same elements.
The Four Coating Families and Their Designations
EN 10346 covers continuously hot-dip coated flat product and uses a letter code followed by a number that gives the coating mass on both surfaces combined, so Z275 is pure zinc at 275 g/m² total. ASTM standards use parallel systems for the same products, with ASTM A653/A653M for zinc, ASTM A1046 for the zinc-5% aluminium family and ASTM A792 for the 55% aluminium-zinc family.
| Coating code | Composition basis | Typical coating masses | Corrosion character |
|---|---|---|---|
| Z | Zinc with normal bath additions | Z100 to Z600 | Barrier plus sacrificial protection, standard reference coating |
| ZA | Zinc with about 5% aluminium | ZA255 and similar | Better than pure zinc in industrial atmospheres and at formed edges |
| AZ | Aluminium with about 55% aluminium and zinc balance | AZ150 and similar | Excellent barrier performance, sensitive to cut-edge exposure |
| ZM | Zinc with roughly 1 to 2% aluminium and 1 to 2% magnesium | ZM120 to ZM430 | Best cut-edge and scratch protection of the four families |
The ZM family is the one usually meant by zinc-aluminum-magnesium coated steel. Magnesium additions in the region of 1% to 2% are what produce the characteristic improvement at sheared edges, drilled holes and scratches, which is where a pure zinc coating loses its effectiveness first.
Grades and Their Meaning
The coating is only half of the specification. The steel substrate is quoted separately, and two designations cause most of the confusion in enquiries.
S350GD is a structural grade under EN 10346 with a minimum yield strength of 350 MPa, delivered hot-dip coated. It is a formed structural material, so it is ordered when the part must carry load as well as resist corrosion.
SGH340 is a Japanese designation under JIS G3302 for hot-dip coated steel sheet for structural use, where 340 is the minimum tensile strength in megapascals. It sits between commercial quality grades and the higher strength structural grades of the same standard.
Commercial forming grades such as DX51D remain the commonest substrate for general enclosure and panel work where formability matters more than strength.
Matching the wrong substrate to the coating designation is a frequent ordering error, because the coating code says nothing about yield strength, elongation or the forming route.
Applications and Where Each Family Fits
Photovoltaic mounting brackets and rails: ZM coatings in the higher mass range perform in C4 and even C5 corrosivity categories where a standard galvanized coating would need a much heavier coating mass to achieve the same life.
Building cladding, roofing and purlins: Z and ZA coatings in the 150 to 275 g/m² range for general construction, with ZM chosen for coastal and industrial roofs.
Automotive and appliance parts: thinner ZM and ZA coatings where cut-edge corrosion resistance in hemmed and pierced sections matters.
Agricultural and outdoor equipment: AZ coatings where a stable barrier layer survives long atmospheric exposure with limited edge exposure.
Forming, Joining and Quality Control
ZM and ZA coatings withstand roll forming and bending well, but severe drawing should be assessed by forming trials because magnesium-bearing coatings are harder than pure zinc at the same mass.
Spot welding of coated sheet requires electrode life management. Coating mass, electrode force and current schedule all influence electrode wear, and weld schedules must be qualified for the specific coating family.
Cut-edge performance is verified by salt spray testing to ISO 9227 and by outdoor exposure arranged to ISO 8565, with time to red rust recorded for the coating mass under evaluation.
Coating mass is confirmed by the gravimetric methods of ISO 1460 or GB/T 1839, and coating adhesion by bend or impact testing as required by the product standard.
State the coating code, coating mass, substrate grade, surface treatment and coil or sheet dimensions on the order, and request an EN 10204 3.1 certificate covering both substrate properties and coating mass.
Frequently Asked Questions
Q: Is zinc-aluminum-magnesium the same as aluminum-zinc coated steel?
A: No. Zinc-aluminum-magnesium is a zinc-based coating with small aluminium and magnesium additions, while aluminum-zinc is an aluminium-based coating with roughly 55% aluminium and a zinc balance. They have different codes and different edge behaviour.
Q: Does a ZM coating replace hot-dip galvanizing?
A: It replaces hot-dip galvanizing in many sheet applications such as photovoltaic brackets and cladding, because it gives comparable or longer life at a much lower coating mass, but it is a continuously coated coil product and is not a substitute for galvanizing heavy fabricated steelwork.
Q: What does S350GD mean?
A: It is a structural steel grade under EN 10346 with a minimum yield strength of 350 MPa, supplied with a hot-dip coating, so it combines load-bearing capacity with corrosion protection.
Q: How much magnesium is needed for better edge protection?
A: Additions of roughly 1% to 2% magnesium with a similar aluminium level are what distinguish the ZM family from pure zinc, and that is the level at which the marked improvement in cut-edge corrosion appears.
Q: Can ZM coated sheet be left unpainted outdoors?
A: Yes, it is used unpainted in many outdoor applications, but where colour and appearance matter the surface is normally coil coated as well, and the coating system is then selected for the atmosphere rather than the metallic coating alone.