What Grain-Oriented Electrical Steel Is
Grain-oriented electrical steel is a silicon steel with a silicon content of about 3%, produced so that the easy magnetisation direction of each grain coincides with the rolling direction. A secondary recrystallisation step in the production route develops this Goss texture, and the result is a material with high magnetic induction and low core loss when the flux path follows the rolling direction and low performance when it does not.
Two consequences follow from that anisotropy. First, the material is only economical in cores where the flux direction is fixed and known, which means laminated cores with the rolling direction aligned to the limbs. Second, the material is supplied with a defined directional property set, and every grade is rated by specific core loss at a stated induction and frequency rather than by a single mechanical value.
Grade Designation and Standardised Properties
Chinese designations under GB/T 2521.1 combine nominal thickness in millimetres with the letter Q for oriented material and a loss figure. A 30Q120 grade is therefore 0.30 mm thick with a maximum specific loss of 1.20 W/kg, and a 35Q155 grade is 0.35 mm thick with a maximum loss of 1.55 W/kg, both measured at 1.7 T and 50 Hz in the standardised test.
The IEC system in IEC 60404-8-7 uses an M prefix with the specific loss expressed as a three-digit number multiplied by a hundredth, followed by the thickness, so an M105-30 grade means 1.05 W/kg at 0.30 mm thickness. Loss values decrease as thickness falls and as grain orientation improves, and the magnetic polarisation at 800 A/m is used to separate conventional grades from high magnetic induction grades.
| Property | Conventional oriented grades | High magnetic induction grades |
|---|---|---|
| Grain texture | Well oriented Goss texture | Sharper Goss texture with improved alignment |
| Magnetic polarisation at 800 A/m | Around 1.80 T and above | Above 1.88 T |
| Core loss at 1.7 T, 50 Hz | Higher, thickness dependent | Lower for the same thickness |
| Typical thickness | 0.30 mm and 0.35 mm | 0.23 mm, 0.27 mm and 0.30 mm |
Main Applications
Power and distribution transformer cores: flux is unidirectional along the limbs and yokes, so the low loss and high induction of the oriented grade directly reduce no-load loss and raise transformer efficiency.
Instrument transformers: current and voltage transformers work at low flux density where stable, low-loss magnetisation gives accurate ratio and phase performance.
Reactors and chokes: gapped cores carry directional flux, and oriented steel with defined lamination stacking controls loss in the gap region.
Large rotating machines with axial flux paths: a limited duty where the direction of magnetisation can be kept aligned during operation.
Where flux rotates, as in the stator and rotor of induction motors and generators, oriented steel is the wrong choice because the rotating flux continually crosses the difficult direction. Non-oriented electrical steel exists precisely for those duties.
Coating, Cutting and Core Building Practice
Oriented strip carries an insulating coating that provides inter-laminar resistance and, in some grades, also the tension that improves magnetic properties. Coating types are designated in the standard, and the coating choice is made with the core building process in mind because some coatings withstand stress relief annealing and some do not.
Burr height after slitting and shearing should be kept as low as practical, typically below 0.02 mm, because burrs create inter-laminar short circuits and increase eddy-current loss.
Cutting introduces local stress that raises loss. Where the process allows, the affected zone is kept away from high flux density regions of the core.
Lamination stacking is done with the rolling direction aligned along the flux path, and mitred joints at the corners are used to preserve flux continuity in wound core construction.
Clamping pressure is controlled because excessive compression degrades magnetic properties, while insufficient pressure causes noise and movement.
Quality Control and Supply Points
Confirm specific core loss, magnetic polarisation and thickness tolerance for each grade, with test data from the production lot rather than a generic table.
Magnetic properties are measured on the Epstein frame per IEC 60404-2 or on a single sheet tester per IEC 60404-3, and the test method should be stated because the two do not give identical values.
Check coating type, coating thickness and inter-laminar resistance, particularly for cores that will be annealed after winding.
Verify flatness and residual curvature, because poor flatness distorts stacked cores and increases building time.
Supply is by coil with a defined slit width and by cut lengths for cores, with material certificates listing grade, heat number and magnetic test results.
Frequently Asked Questions
Q: Why is grain-oriented steel not used in electric motors?
A: Motor cores carry rotating flux that sweeps across the difficult magnetisation direction, so the low loss advantage disappears and non-oriented electrical steel gives better overall performance.
Q: What does the number in 30Q120 mean?
A: The 30 gives the nominal thickness in hundredths of a millimetre, so 0.30 mm, and 120 gives the maximum specific core loss multiplied by one hundred, so 1.20 W/kg at the standardised test condition.
Q: What is the difference between conventional and high magnetic induction oriented steel?
A: High magnetic induction grades have a sharper grain orientation, giving a magnetic polarisation above 1.88 T at 800 A/m against roughly 1.80 T for conventional grades, which reduces core size and loss for the same transformer rating.
Q: Does the insulating coating matter for performance?
A: It does. The coating controls inter-laminar resistance and therefore eddy-current loss, and in tension-coated grades it also improves magnetic properties, so the coating type must be matched to the annealing and building route.
Q: How should oriented strip be stored?
A: Indoors in a dry, ventilated area with the coil axis horizontal, off the floor and free from condensation, because edge rust and moisture damage degrade the surface insulation and are not recoverable by processing.